EN 12591:2009
European product standards cover a large variety of road materials for different applications, to accommodate local traffic loads and climate conditions. This European standard therefore also covers a large range of bitumens to facilitate the production and application of the designed paving. The variety of production techniques and applications makes it more practical to split bitumens into 20/30, 30/45, 35/50, 40/60, 50/70, 70/100, 100/150, 160/220. Fouman Chimie Gostar is capable of producing the following grades:
Characteristic
|
Unit
|
35-50
|
Test Method
|
Penetration @ 25 °C
|
dmm
|
35-50
|
EN 1426
|
Softening Point
|
°C
|
50-58
|
EN 1427
|
Resistance to Hardening @163 °C:
Retained Penetration
Change of Mass
|
%
%
|
53 min
0.5 max
|
EN 12607-1
|
Flash Point
|
°C
|
240 min
|
EN ISO 2592
|
Solubility
|
%
|
99.0 min
|
EN 12592
|
Penetration Index
|
-
|
-1.5 to +0.7
|
EN 12591-Annex A
|
Dynamic Viscosity @ 60 °C
|
Pa.S
|
225 min
|
EN 12596
|
Fraass Breaking Point
|
°C
|
-5 max
|
EN 12593
|
Kinematic Viscosity @ 135 °C
|
cSt
|
370 min
|
EN 12595
|
Characteristic
|
Unit
|
50-70
|
Test Method
|
Penetration @ 25 °C
|
dmm
|
50-70
|
EN 1426
|
Softening Point
|
°C
|
46-54
|
EN 1427
|
Resistance to Hardening @163 °C:
Retained Penetration
Change of Mass
|
%
%
|
50 min
0.5 max
|
EN 12607-1
|
Flash Point
|
°C
|
230 min
|
EN ISO 2592
|
Solubility
|
%
|
99.0 min
|
EN 12592
|
Penetration Index
|
-
|
-1.5 to +0.7
|
EN 12591-Annex A
|
Dynamic Viscosity @ 60 °C
|
Pa.S
|
145 min
|
EN 12596
|
Fraass Breaking Point
|
°C
|
-8 max
|
EN 12593
|
Kinematic Viscosity @ 135 °C
|
cSt
|
295 min
|
EN 12595
|
Characteristic
|
Unit
|
70-100
|
Test Method
|
Penetration @ 25 °C
|
dmm
|
70-100
|
EN 1426
|
Softening Point
|
°C
|
43-51
|
EN 1427
|
Resistance to Hardening @163 °C:
Retained Penetration
Change of Mass
|
%
%
|
46 min
0.8 max
|
EN 12607-1
|
Flash Point
|
°C
|
230 min
|
EN ISO 2592
|
Solubility
|
%
|
99.0 min
|
EN 12592
|
Penetration Index
|
-
|
-1.5 to +0.7
|
EN 12591-Annex A
|
Dynamic Viscosity @ 60 °C
|
Pa.S
|
90 min
|
EN 12596
|
Fraass Breaking Point
|
°C
|
-10 max
|
EN 12593
|
Kinematic Viscosity @ 135 °C
|
cSt
|
230 min
|
EN 12595
|
Characteristic
|
Unit
|
100-150
|
Test Method
|
Penetration @ 25 °C
|
dmm
|
100-150
|
EN 1426
|
Softening Point
|
°C
|
39-47
|
EN 1427
|
Resistance to Hardening @163 °C:
Retained Penetration
Change of Mass
|
%
%
|
43 min
0.8 max
|
EN 12607-1
|
Flash Point
|
°C
|
230 min
|
EN ISO 2592
|
Solubility
|
%
|
99.0 min
|
EN 12592
|
Penetration Index
|
-
|
-1.5 to +0.7
|
EN 12591-Annex A
|
Dynamic Viscosity @ 60 °C
|
Pa.S
|
55 min
|
EN 12596
|
Fraass Breaking Point
|
°C
|
-12 max
|
EN 12593
|
Kinematic Viscosity @ 135 °C
|
cSt
|
175 min
|
EN 12595
|
Characteristic
|
Unit
|
160-220
|
Test Method
|
Penetration @ 25 °C
|
dmm
|
160-220
|
EN 1426
|
Softening Point
|
°C
|
35-43
|
EN 1427
|
Resistance to Hardening @163 °C:
Retained Penetration
Change of Mass
|
%
%
|
37 min
1.0 max
|
EN 12607-1
|
Flash Point
|
°C
|
220 min
|
EN ISO 2592
|
Solubility
|
%
|
99.0 min
|
EN 12592
|
Penetration Index
|
-
|
-1.5 to +0.7
|
EN 12591-Annex A
|
Dynamic Viscosity @ 60 °C
|
Pa.S
|
30 min
|
EN 12596
|
Fraass Breaking Point
|
°C
|
-15 max
|
EN 12593
|
Kinematic Viscosity @ 135 °C
|
cSt
|
135 min
|
EN 12595
|